| Nominal Size (mm) | Schedule no. | Wall Thickness (mm) | Maximum Allowable Pressure (kPa) | ||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| Temperature (oC) | |||||||||||
| -29 - 38 | 205 | 260 | 350 | 370 | 400 | 4301) | 450 | ||||
| Maximum Allowable Stress (MPa) | |||||||||||
| 137.8 | 137.8 | 130.2 | 117.1 | 115.7 | 89.6 | 74.4 | 59.9 | ||||
| 15 | STD | 40 | 2.77 | 34416 | 34416 | 32528 | 29255 | 28910 | 22372 | 18589 | 14972 |
| XS | 80 | 3.73 | 48092 | 48092 | 45466 | 40878 | 40396 | 31260 | 25969 | 20918 | |
| 160 | 4.78 | 62830 | 62830 | 59378 | 53404 | 52777 | 40837 | 33929 | 27333 | ||
| XXS | 7.47 | 98245 | 98245 | 92836 | 83507 | 82522 | 63857 | 53053 | 42739 | ||
| 20 | STD | 40 | 2.87 | 28070 | 28070 | 26526 | 23860 | 23578 | 18245 | 15158 | 12209 |
| XS | 80 | 3.91 | 39418 | 39418 | 37247 | 33506 | 33106 | 25617 | 21283 | 17142 | |
| 160 | 5.56 | 58152 | 58152 | 54955 | 49429 | 48843 | 37799 | 31398 | 25293 | ||
| XXS | 7.82 | 83107 | 83107 | 78539 | 70643 | 69809 | 54024 | 44881 | 36152 | ||
| 25 | STD | 40 | 3.38 | 26251 | 26251 | 24804 | 22310 | 22048 | 17060 | 14173 | 11417 |
| XS | 80 | 4.55 | 36283 | 36283 | 34285 | 30862 | 30474 | 23584 | 19595 | 15785 | |
| 160 | 6.35 | 52481 | 52481 | 49594 | 44606 | 44082 | 34112 | 28339 | 22827 | ||
| XXS | 9.09 | 77030 | 77030 | 72793 | 65476 | 64704 | 50070 | 41595 | 33506 | ||
| 32 | STD | 40 | 3.56 | 21614 | 21614 | 20421 | 18369 | 18155 | 14049 | 11672 | 9404 |
| XS | 80 | 4.85 | 30178 | 30178 | 28518 | 25651 | 25348 | 19616 | 16295 | 13125 | |
| 160 | 6.35 | 40596 | 40596 | 38364 | 34505 | 34099 | 26389 | 21924 | 17659 | ||
| XXS | 9.70 | 64601 | 64601 | 61045 | 54906 | 54266 | 41988 | 34884 | 28097 | ||
| 40 | STD | 40 | 3.68 | 19444 | 19444 | 18375 | 16529 | 16329 | 12636 | 10550 | 8454 |
| XS | 80 | 5.08 | 27402 | 27402 | 25900 | 23295 | 23019 | 17811 | 14800 | 11919 | |
| 160 | 7.14 | 39738 | 39738 | 37599 | 33816 | 33416 | 25858 | 21483 | 17308 | ||
| XXS | 10.16 | 58779 | 58799 | 55547 | 49966 | 49374 | 38205 | 31742 | 25569 | ||
| 50 | STD | 40 | 3.91 | 16378 | 16378 | 15468 | 13925 | 13759 | 10645 | 8847 | 7124 |
| XS | 80 | 5.54 | 23653 | 23653 | 22351 | 20105 | 19871 | 15378 | 12774 | 10287 | |
| 160 | 8.74 | 38866 | 38866 | 36731 | 33037 | 32652 | 25266 | 20987 | 16908 | ||
| XXS | 11.07 | 50793 | 50793 | 48003 | 43173 | 42670 | 33017 | 27429 | 22096 | ||
| 65 | STD | 40 | 5.16 | 17914 | 17914 | 16929 | 15227 | 15048 | 11644 | 9674 | 7793 |
| XS | 80 | 7.01 | 24818 | 24818 | 23447 | 21097 | 20849 | 16129 | 13401 | 10797 | |
| 160 | 9.53 | 34615 | 34615 | 32714 | 29420 | 29076 | 22503 | 18693 | 15055 | ||
| XXS | 14.02 | 53081 | 53081 | 50159 | 45116 | 44585 | 34498 | 28662 | 23088 | ||
| 80 | STD | 40 | 5.49 | 15558 | 15558 | 14969 | 13222 | 13063 | 10108 | 8399 | 6766 |
| XS | 80 | 7.62 | 21986 | 21968 | 20780 | 18693 | 18472 | 14290 | 11871 | 9563 | |
| 160 | 11.13 | 33079 | 33079 | 31253 | 28111 | 27780 | 21497 | 17859 | 14386 | ||
| XXS | 15.24 | 46976 | 46976 | 44392 | 39928 | 39459 | 30536 | 25369 | 20436 | ||
| 100 | STD | 40 | 6.02 | 13187 | 13187 | 12464 | 11210 | 11079 | 8571 | 7124 | 5739 |
| XS | 80 | 8.56 | 19058 | 19058 | 18010 | 16198 | 16012 | 12388 | 12094 | 8289 | |
| 120 | 11.13 | 25190 | 25190 | 23805 | 21407 | 21159 | 16371 | 13601 | 10995 | ||
| 160 | 13.49 | 31019 | 31019 | 29310 | 26368 | 26058 | 20160 | 16750 | 13208 | ||
| XXS | 17.12 | 40348 | 40348 | 38129 | 34298 | 33892 | 26230 | 21786 | 17549 | ||
| 125 | STD | 40 | 6.55 | 11561 | 11561 | 10921 | 9825 | 9708 | 7510 | 6243 | 5038 |
| XS | 80 | 9.53 | 17060 | 17060 | 16122 | 14503 | 14331 | 11093 | 9212 | 7421 | |
| 120 | 12.70 | 23130 | 23130 | 21855 | 19657 | 19430 | 15034 | 12492 | 10059 | ||
| 160 | 15.88 | 29407 | 29407 | 27787 | 24997 | 24701 | 19113 | 15881 | 12795 | ||
| XXS | 19.05 | 35897 | 35897 | 33926 | 30516 | 30158 | 23337 | 19388 | 15620 | ||
| 150 | STD | 40 | 7.11 | 10550 | 10550 | 9928 | 8924 | 8819 | 6828 | 5370 | 4568 |
| XS | 80 | 10.97 | 16474 | 16474 | 15571 | 14007 | 13842 | 10707 | 8895 | 7165 | |
| 120 | 14.27 | 21745 | 21745 | 20553 | 18448 | 18265 | 14138 | 11747 | 9460 | ||
| XXS | 160 | 18.26 | 28325 | 28325 | 26768 | 24074 | 23784 | 18410 | 15296 | 12319 | |
| 200 | 20 | 6.35 | 7138 | 7138 | 6745 | 6063 | 5994 | 4637 | 3852 | 3100 | |
| 30 | 7.04 | 7924 | 7924 | 7489 | 6732 | 6656 | 5147 | 4279 | 3445 | ||
| STD | 40 | 8.18 | 9246 | 9246 | 8737 | 7855 | 7765 | 6008 | 4995 | 4024 | |
| 60 | 10.31 | 11741 | 11741 | 11093 | 9977 | 9860 | 7627 | 6339 | 5105 | ||
| XS | 80 | 12.70 | 14572 | 14572 | 13766 | 12388 | 12237 | 9474 | 7868 | 6338 | |
| 100 | 15.09 | 17452 | 17452 | 16488 | 14834 | 14655 | 11341 | 9426 | 7593 | ||
| 120 | 18.26 | 21345 | 21345 | 20174 | 18148 | 17935 | 13876 | 11527 | 9288 | ||
| 140 | 20.62 | 24308 | 24308 | 22971 | 20656 | 20415 | 15799 | 13125 | 10569 | ||
| XXS | 22.23 | 26334 | 26334 | 24877 | 22386 | 22124 | 17115 | 14221 | 11458 | ||
| 160 | 23.01 | 27340 | 27340 | 25838 | 23240 | 22964 | 17769 | 14765 | 11892 | ||
| 250 | 20 | 6.35 | 5698 | 5698 | 5388 | 4844 | 4789 | 3707 | 3080 | 2480 | |
| 30 | 7.8 | 7028 | 7028 | 6642 | 5974 | 5905 | 4568 | 3796 | 3059 | ||
| STD | 40 | 9.27 | 8385 | 8385 | 7923 | 7131 | 7048 | 5450 | 4527 | 3652 | |
| XS | 60 | 12.7 | 11596 | 11596 | 10955 | 9853 | 9736 | 7538 | 6263 | 5043 | |
| 80 | 15.09 | 13863 | 13863 | 13098 | 11781 | 11644 | 9012 | 7483 | 6028 | ||
| 100 | 18.26 | 16922 | 16922 | 15992 | 14386 | 14214 | 10996 | 9136 | 7359 | ||
| 120 | 21.44 | 20036 | 20036 | 18934 | 17032 | 16825 | 13022 | 10817 | 8716 | ||
| XXS | 140 | 25.4 | 23998 | 23998 | 16474 | 20394 | 20153 | 15599 | 12960 | 10438 | |
| 160 | 28.58 | 27229 | 27229 | 25734 | 23143 | 22875 | 17700 | 14703 | 11844 | ||
| 300 | 20 | 6.35 | 4795 | 4795 | 4534 | 4072 | 4024 | 3114 | 2591 | 2088 | |
| 30 | 8.38 | 6359 | 6359 | 6008 | 5402 | 5540 | 4134 | 3431 | 2763 | ||
| STD | 9.53 | 7241 | 7241 | 6842 | 6153 | 6084 | 4706 | 3914 | 3149 | ||
| 40 | 10.31 | 7854 | 7854 | 7421 | 6676 | 6601 | 5015 | 4244 | 3417 | ||
| XS | 12.70 | 9722 | 9722 | 9191 | 8268 | 8165 | 6318 | 5250 | 4230 | ||
| 60 | 14.27 | 10969 | 10969 | 10363 | 9322 | 9212 | 7131 | 5925 | 4768 | ||
| 80 | 17.48 | 13525 | 13525 | 12850 | 11492 | 11362 | 8792 | 7303 | 5884 | ||
| 100 | 21.44 | 16736 | 16736 | 15819 | 14227 | 14062 | 10879 | 9040 | 7283 | ||
| XXS | 120 | 25.4 | 20015 | 20015 | 18913 | 17011 | 16811 | 13008 | 10804 | 8702 | |
| 140 | 28.58 | 22682 | 22682 | 21435 | 19278 | 19051 | 14744 | 12244 | 9866 | ||
| 160 | 33.32 | 26740 | 26740 | 25273 | 22730 | 22461 | 17383 | 14441 | 11630 | ||
| 350 | 10 | 6.35 | 4361 | 4361 | 4120 | 3707 | 3665 | 2831 | 2356 | 1895 | |
| 20 | 7.92 | 5457 | 5457 | 5161 | 4644 | 4589 | 3548 | 2949 | 2377 | ||
| STD | 30 | 9.53 | 6580 | 6580 | 6222 | 5595 | 5533 | 4279 | 3555 | 2866 | |
| 40 | 11.13 | 7717 | 7717 | 7310 | 6559 | 6477 | 5016 | 4168 | 3355 | ||
| XS | 12.70 | 8833 | 8833 | 8351 | 7510 | 7421 | 5739 | 4768 | 3845 | ||
| 60 | 15.09 | 10541 | 10541 | 9963 | 8964 | 8861 | 6855 | 5691 | 4589 | ||
| 80 | 19.05 | 13421 | 13421 | 12684 | 11410 | 11272 | 9723 | 7248 | 5836 | ||
| 100 | 23.83 | 16949 | 16949 | 16019 | 14407 | 14242 | 11017 | 9157 | 7372 | ||
| 120 | 27.79 | 19933 | 19933 | 18837 | 16943 | 16743 | 12960 | 10762 | 8675 | ||
| 140 | 31.75 | 22964 | 22964 | 21703 | 19519 | 19292 | 14931 | 12402 | 9990 | ||
| 160 | 35.71 | 26051 | 26051 | 24618 | 22144 | 21883 | 16936 | 14069 | 11334 | ||
| 400 | 10 | 6.35 | 3810 | 3810 | 3603 | 3238 | 3197 | 2474 | 2060 | 1660 | |
| 20 | 7.92 | 4768 | 4768 | 4507 | 4051 | 4004 | 3100 | 2577 | 2074 | ||
| STD | 30 | 9.53 | 5746 | 5746 | 5429 | 4885 | 4830 | 3734 | 3100 | 2501 | |
| XS | 40 | 12.70 | 7703 | 7703 | 7283 | 6545 | 6470 | 5009 | 4126 | 3349 | |
| 60 | 16.66 | 10176 | 10176 | 9618 | 8654 | 8550 | 6614 | 5498 | 4430 | ||
| 80 | 21.44 | 13208 | 13208 | 12478 | 11224 | 11093 | 8585 | 7131 | 5746 | ||
| 100 | 26.19 | 16274 | 16274 | 15378 | 13835 | 13670 | 10576 | 8785 | 7076 | ||
| 120 | 30.96 | 19409 | 19409 | 18341 | 16481 | 16302 | 12616 | 10480 | 8440 | ||
| 140 | 36.53 | 23130 | 23130 | 21855 | 19657 | 19430 | 15034 | 12492 | 10059 | ||
| 160 | 40.49 | 25824 | 25824 | 24404 | 21952 | 21697 | 16784 | 13945 | 11238 | ||
| 450 | 10 | 6.35 | 3383 | 3383 | 3197 | 2873 | 2839 | 2198 | 1826 | 1474 | |
| 20 | 7.92 | 4230 | 4230 | 3996 | 3597 | 3555 | 2749 | 2287 | 1839 | ||
| STD | 9.53 | 5099 | 5099 | 4816 | 4334 | 4286 | 3314 | 2756 | 2219 | ||
| XS | 30 | 11.13 | 5967 | 5967 | 5643 | 5071 | 5016 | 3879 | 3225 | 2598 | |
| 12.70 | 6835 | 6835 | 6456 | 5808 | 5739 | 4437 | 3686 | 2969 | |||
| 40 | 14.27 | 7696 | 7696 | 7276 | 6545 | 6463 | 5002 | 4155 | 3349 | ||
| 60 | 19.05 | 10349 | 10349 | 9784 | 8799 | 8695 | 6725 | 5588 | 4499 | ||
| 80 | 23.83 | 13043 | 13043 | 12326 | 11086 | 10955 | 8475 | 7042 | 5670 | ||
| 100 | 29.36 | 16219 | 16219 | 15323 | 13787 | 13622 | 10542 | 8757 | 7055 | ||
| 120 | 34.93 | 19464 | 19464 | 18389 | 16543 | 16350 | 12650 | 10507 | 8468 | ||
| 140 | 39.67 | 22282 | 22282 | 21056 | 18941 | 18713 | 11483 | 12030 | 9694 | ||
| 160 | 45.24 | 25638 | 25638 | 24225 | 21793 | 21531 | 16660 | 13842 | 11155 | ||
| 500 | 10 | 6.35 | 3038 | 3038 | 2873 | 2574 | 2556 | 1977 | 1640 | 1323 | |
| STD | 20 | 9.53 | 4582 | 4582 | 4327 | 3893 | 3852 | 2976 | 2474 | 1991 | |
| XS | 30 | 12.70 | 6139 | 6139 | 5801 | 5216 | 5154 | 3989 | 3314 | 2666 | |
| 40 | 15.09 | 7317 | 7317 | 6911 | 6215 | 6146 | 4754 | 3948 | 3183 | ||
| 60 | 20.62 | 10080 | 10080 | 9522 | 8564 | 8468 | 6552 | 5443 | 4382 | ||
| 80 | 26.19 | 12898 | 12898 | 12188 | 10962 | 10831 | 8385 | 6966 | 5608 | ||
| 100 | 32.54 | 16171 | 16171 | 15287 | 13746 | 13580 | 10514 | 8730 | 7035 | ||
| 120 | 38.10 | 19085 | 19085 | 18037 | 16226 | 16033 | 12409 | 10307 | 8302 | ||
| 140 | 44.45 | 22475 | 22475 | 21242 | 19106 | 18879 | 14614 | 12140 | 9777 | ||
| 160 | 50.01 | 25450 | 25450 | 24094 | 21675 | 21421 | 16577 | 13766 | 11093 | ||
| 600 | 10 | 6.35 | 2529 | 2529 | 2391 | 2150 | 2129 | 1647 | 1364 | 1102 | |
| STD | 20 | 9.53 | 3810 | 3810 | 3603 | 3238 | 3197 | 2474 | 2060 | 1660 | |
| XS | 12.70 | 5097 | 5097 | 4816 | 4334 | 4286 | 3314 | 2756 | 2219 | ||
| 30 | 14.27 | 5739 | 5739 | 5423 | 4878 | 4823 | 3734 | 3100 | 2494 | ||
| 40 | 17.48 | 7055 | 7055 | 6670 | 5994 | 5925 | 4589 | 3810 | 3066 | ||
| 60 | 24.61 | 10018 | 10018 | 9467 | 8516 | 8420 | 6511 | 5409 | 4361 | ||
| 80 | 30.96 | 12691 | 12691 | 12002 | 10783 | 10659 | 8254 | 6856 | 5519 | ||
| 100 | 38.89 | 16102 | 16102 | 15220 | 13690 | 10528 | 10466 | 8695 | 7007 | ||
| 120 | 46.02 | 19223 | 19223 | 18168 | 16336 | 16150 | 12491 | 10383 | 8364 | ||
| 140 | 52.37 | 22048 | 22048 | 20835 | 18741 | 18520 | 14331 | 11906 | 9591 | ||
| 160 | 59.54 | 25279 | 25279 | 23888 | 21489 | 21235 | 16433 | 13649 | 10996 | ||
1) Due to the possible conversion of carbon to graphite (graphitization) - carbon steel pipes should be avoided for temperatures above 425 oC. Instead Alloy steels should be used.
- 1 MPa = 106 N/m2
- Calculations are made with the Barlow's Formula
Related Topics
• Pressure Ratings of Pipes and Fittings
Pressure ratings of pipes and tubes and their fittings - carbon steel , stainless steel, plastic, copper and more.
Related Documents
ANSI B16.5 - Steel Pipe Flanges - Pressure and Temperature Ratings - Group 1.2.
Pressure (psig) and temperature ratings for steel pipe flanges and flanged fittings
API - American Petroleum Institute
The American Petroleum Institute - API.
ASME 31.3 Piping Materials - Allowable Pressure Calculator
Calculate ASME 31.3 allowable pressure
ASME B31 Pressure Piping - Overview
A survey of one of the most important pressure pipe codes - ASME B31, earlier known as ANSI B31.
ASME B31.9 Building Services Piping - Working Pressure and Temperature Limits
The working pressure and temperature limits of ASME Code B31.9 - Building Services Piping.
ASME/ANSI B36.10/19 - Carbon, Alloy and Stainless Steel Pipe - Dimensions
Pipe sizes, inside and outside diameters, wall thickness, schedules, moment of inertia, transverse area, weight of pipe filled with water - U.S. Customary Units.
ASTM A312 Stainless Steel Pipes - Bursting and Collapsing Pressures
Theoretic bursting and collapsing pressures for stainless steel pipes ASTM A312.
ASTM A53 B Carbon Steel Pipes - Allowable Pressure vs. Schedule and Size
Maximum working pressure of carbon steel pipe at temperature 400oF.
Barlow's Formula - Calculate Internal, Allowable and Bursting Pressure
Calculate pipes internal, allowable and bursting pressure.
Carbon Steel Flanges - Group 1.1 Pressure and Temperature Ratings
Maximum temperature and pressure ratings of flanges conforming dimensions ASME B16.5 and materials specification ASTM A-105.
Carbon Steel Pipes - Pressure and Temperature Ratings, Imperial Units
Pressure (psig) and temperature (deg F) ratings for A-53 B and A-106 B, A333, A334 and API 5L carbon steel pipes - temperatures ranging 100 degF - 700 degF.
PN Pressure Ratings for Flanges: Specifications & Standards
Pressure numbers (PN) vs. flange class designations.
Process Pipes - Allowable Stress vs. Temperature
Allowable wall stress in pipes according ASME M31.3.
Schedule - Terminology
Introduction to the schedule terminology of pipes.
Stainless Steel Pipes - Allowable Pressure vs. Schedule and Size
Allowable pressure for standard seamless A312-TP316/316L stainless steel pipes - temperatures 100oF to 750oF.
Steel Pipes - De-Rating vs. Temperature
Temperature derating factor for steel pipes.
Wrought Steel Pipes - Bursting Pressures vs. Size
Theoretical bursting and working pressure of wrought steel standard, extra strong and double extra strong pipes.