Solids, Liquids and Gases - Thermal Conductivities
Thermal conductivity coefficients for insulation materials, aluminum, asphalt, brass, copper, steel, gases and more.
Thermal conductivity is a material property that describes ability to conduct heat . Thermal conductivity can be defined as
"the quantity of heat transmitted through a unit thickness of a material - in a direction normal to a surface of unit area - due to a unit temperature gradient under steady state conditions"
Thermal conductivity units are [W/(m K)] in the SI system and [Btu/(hr ft °F)] in the Imperial system.
See also thermal conductivity variations with temperature and pressure , for: Air , Ammonia , Carbon Dioxide and Water
Thermal conductivities for common materials and products:
Material/Substance | Thermal Conductivity - k - W/(m K) | ||
---|---|---|---|
Temperature | |||
25 o C (77 o F) | 125 o C (257 o F) | 225 o C (437 o F) | |
Acetals | 0.23 | ||
Acetals | 0.23 | ||
Acetone | 0.16 | ||
Acetylene (gas) | 0.018 | ||
Acrylic | 0.2 | ||
Air, atmosphere (gas) | 0.0262 | 0.0333 | 0.0398 |
Air, elevation 10000 m | 0.020 | ||
Agate | 10.9 | ||
Alcohol | 0.17 | ||
Alumina | 36 | 26 | |
Aluminum | |||
Aluminum Brass | 121 | ||
Aluminum Oxide | 30 | ||
Ammonia (gas) | 0.0249 | 0.0369 | 0.0528 |
Antimony | 18.5 | ||
Apple (85.6% moisture) | 0.39 | ||
Argon (gas) | 0.016 | ||
Asbestos-cement board 1) | 0.744 | ||
Asbestos-cement sheets 1) | 0.166 | ||
Asbestos-cement 1) | 2.07 | ||
Asbestos, loosely packed 1) | 0.15 | ||
Asbestos mill board 1) | 0.14 | ||
Asphalt | 0.75 | ||
Balsa wood | 0.048 | ||
Bitumen | 0.17 | ||
Bitumen/felt layers | 0.5 | ||
Beef, lean (78.9 % moisture) | 0.43 - 0.48 | ||
Benzene | 0.16 | ||
Beryllium | |||
Bismuth | 8.1 | ||
Bitumen | 0.17 | ||
Blast furnace gas (gas) | 0.02 | ||
Boiler scale | 1.2 - 3.5 | ||
Boron | 25 | ||
Brass | |||
Breeze block | 0.10 - 0.20 | ||
Brick dense | 1.31 | ||
Brick, fire | 0.47 | ||
Brick, insulating | 0.15 | ||
Brickwork, common (Building Brick) | 0.6 -1.0 | ||
Brickwork, dense | 1.6 | ||
Bromine (gas) | 0.004 | ||
Bronze | |||
Brown iron ore | 0.58 | ||
Butter (15% moisture content) | 0.20 | ||
Cadmium | |||
Calcium silicate | 0.05 | ||
Carbon | 1.7 | ||
Carbon dioxide (gas) | 0.0146 | ||
Carbon monoxide | 0.0232 | ||
Cast iron | |||
Cellulose, cotton, wood pulp and regenerated | 0.23 | ||
Cellulose acetate, molded, sheet | 0.17 - 0.33 | ||
Cellulose nitrate, celluloid | 0.12 - 0.21 | ||
Cement, Portland | 0.29 | ||
Cement, mortar | 1.73 | ||
Ceramic materials | |||
Chalk | 0.09 | ||
Charcoal | 0.084 | ||
Chlorinated poly-ether | 0.13 | ||
Chlorine (gas) | 0.0081 | ||
Chrome Nickel Steel | 16.3 | ||
Chromium | |||
Chrom-oxide | 0.42 | ||
Clay, dry to moist | 0.15 - 1.8 | ||
Clay, saturated | 0.6 - 2.5 | ||
Coal | 0.2 | ||
Cobalt | |||
Cod (83% moisture content) | 0.54 | ||
Coke | 0.184 | ||
Concrete, lightweight | 0.1 - 0.3 | ||
Concrete, medium | 0.4 - 0.7 | ||
Concrete, dense | 1.0 - 1.8 | ||
Concrete, stone | 1.7 | ||
Constantan | 23.3 | ||
Copper | |||
Corian (ceramic filled) | 1.06 | ||
Cork board | 0.043 | ||
Cork, re-granulated | 0.044 | ||
Cork | 0.07 | ||
Cotton | 0.04 | ||
Cotton wool | 0.029 | ||
Carbon Steel | |||
Cotton Wool insulation | 0.029 | ||
Cupronickel 30% | 30 | ||
Diamond | 1000 | ||
Diatomaceous earth (Sil-o-cel) | 0.06 | ||
Diatomite | 0.12 | ||
Duralium | |||
Earth, dry | 1.5 | ||
Ebonite | 0.17 | ||
Emery | 11.6 | ||
Engine Oil | 0.15 | ||
Ethane (gas) | 0.018 | ||
Ether | 0.14 | ||
Ethylene (gas) | 0.017 | ||
Epoxy | 0.35 | ||
Ethylene glycol | 0.25 | ||
Feathers | 0.034 | ||
Felt insulation | 0.04 | ||
Fiberglass | 0.04 | ||
Fiber insulating board | 0.048 | ||
Fiber hardboard | 0.2 | ||
Fire-clay brick 500 o C | 1.4 | ||
Fluorine (gas) | 0.0254 | ||
Foam glass | 0.045 | ||
Dichlorodifluoromethane R-12 (gas) | 0.007 | ||
Dichlorodifluoromethane R-12 (liquid) | 0.09 | ||
Gasoline | 0.15 | ||
Glass | 1.05 | ||
Glass, Pearls, dry | 0.18 | ||
Glass, Pearls, saturated | 0.76 | ||
Glass, window | 0.96 | ||
Glass, wool Insulation | 0.04 | ||
Glycerol | 0.28 | ||
Gold | |||
Granite | 1.7 - 4.0 | ||
Graphite | 168 | ||
Gravel | 0.7 | ||
Ground or soil, very moist area | 1.4 | ||
Ground or soil, moist area | 1.0 | ||
Ground or soil, dry area | 0.5 | ||
Ground or soil, very dry area | 0.33 | ||
Gypsum board | 0.17 | ||
Hairfelt | 0.05 | ||
Hardboard high density | 0.15 | ||
Hardwoods (oak, maple..) | 0.16 | ||
Hastelloy C | 12 | ||
Helium (gas) | 0.142 | ||
Honey (12.6% moisture content) | 0.5 | ||
Hydrochloric acid (gas) | 0.013 | ||
Hydrogen (gas) | 0.168 | ||
Hydrogen sulfide (gas) | 0.013 | ||
Ice (0 o C, 32 o F) | 2.18 | ||
Inconel | 15 | ||
Ingot iron | 47 - 58 | ||
Insulation materials | 0.035 - 0.16 | ||
Iodine | 0.44 | ||
Iridium | 147 | ||
Iron | |||
Iron-oxide | 0.58 | ||
Kapok insulation | 0.034 | ||
Kerosene | 0.15 | ||
Krypton (gas) | 0.0088 | ||
Lead | |||
Leather, dry | 0.14 | ||
Limestone | 1.26 - 1.33 | ||
Lithium | |||
Magnesia insulation (85%) | 0.07 | ||
Magnesite | 4.15 | ||
Magnesium | |||
Magnesium alloy | 70 - 145 | ||
Marble | 2.08 - 2.94 | ||
Mercury, liquid | |||
Methane (gas) | 0.030 | ||
Methanol | 0.21 | ||
Mica | 0.71 | ||
Milk | 0.53 | ||
Mineral wool insulation materials, wool blankets .. | 0.04 | ||
Molybdenum | |||
Monel | |||
Neon (gas) | 0.046 | ||
Neoprene | 0.05 | ||
Nickel | |||
Nitric oxide (gas) | 0.0238 | ||
Nitrogen (gas) | 0.024 | ||
Nitrous oxide (gas) | 0.0151 | ||
Nylon 6, Nylon 6/6 | 0.25 | ||
Oil, machine lubricating SAE 50 | 0.15 | ||
Olive oil | 0.17 | ||
Oxygen (gas) | 0.024 | ||
Palladium | 70.9 | ||
Paper | 0.05 | ||
Paraffin Wax | 0.25 | ||
Peat | 0.08 | ||
Perlite, atmospheric pressure | 0.031 | ||
Perlite, vacuum | 0.00137 | ||
Phenolic cast resins | 0.15 | ||
Phenol-formaldehyde moulding compounds | 0.13 - 0.25 | ||
Phosphorbronze | 110 | ||
Pinchbeck | 159 | ||
Pitch | 0.13 | ||
Pit coal | 0.24 | ||
Plaster light | 0.2 | ||
Plaster, metal lath | 0.47 | ||
Plaster, sand | 0.71 | ||
Plaster, wood lath | 0.28 | ||
Plasticine | 0.65 - 0.8 | ||
Plastics, foamed (insulation materials) | 0.03 | ||
Platinum | |||
Plutonium | |||
Plywood | 0.13 | ||
Polycarbonate | 0.19 | ||
Polyester | 0.05 | ||
Polyethylene low density, PEL | 0.33 | ||
Polyethylene high density, PEH | 0.42 - 0.51 | ||
Polyisoprene natural rubber | 0.13 | ||
Polyisoprene hard rubber | 0.16 | ||
Polymethylmethacrylate | 0.17 - 0.25 | ||
Polypropylene, PP | 0.1 - 0.22 | ||
Polystyrene, expanded | 0.03 | ||
Polystyrol | 0.043 | ||
Polyurethane foam | 0.03 | ||
Porcelain | 1.5 | ||
Potassium | 1 | ||
Potato, raw flesh | 0.55 | ||
Propane (gas) | 0.015 | ||
Polytetrafluoroethylene (PTFE) | 0.25 | ||
Polyvinylchloride, PVC | 0.19 | ||
Pyrex glass | 1.005 | ||
Quartz mineral | 3 | ||
Radon (gas) | 0.0033 | ||
Red metal | |||
Rhenium | |||
Rhodium | |||
Rock, solid | 2 - 7 | ||
Rock, porous volcanic (Tuff) | 0.5 - 2.5 | ||
Rock Wool insulation | 0.045 | ||
Rosin | 0.32 | ||
Rubber, cellular | 0.045 | ||
Rubber, natural | 0.13 | ||
Rubidium | |||
Salmon (73% moisture content) | 0.50 | ||
Sand, dry | 0.15 - 0.25 | ||
Sand, moist | 0.25 - 2 | ||
Sand, saturated | 2 - 4 | ||
Sandstone | 1.7 | ||
Sawdust | 0.08 | ||
Selenium | |||
Sheep wool | 0.039 | ||
Silica aerogel | 0.02 | ||
Silicon cast resin | 0.15 - 0.32 | ||
Silicon carbide | 120 | ||
Silicon oil | 0.1 | ||
Silver | |||
Slag wool | 0.042 | ||
Slate | 2.01 | ||
Snow (temp < 0 o C) | 0.05 - 0.25 | ||
Sodium | |||
Softwoods (fir, pine ..) | 0.12 | ||
Soil, clay | 1.1 | ||
Soil, with organic matter | 0.15 - 2 | ||
Soil, saturated | 0.6 - 4 | ||
Solder 50-50 | 50 | ||
Soot | 0.07 | ||
Steam, saturated | 0.0184 | ||
Steam, low pressure | 0.0188 | ||
Steatite | 2 | ||
Steel, Carbon | |||
Steel, Stainless | |||
Straw slab insulation, compressed | 0.09 | ||
Styrofoam | 0.033 | ||
Sulfur dioxide (gas) | 0.0086 | ||
Sulfur, crystal | 0.2 | ||
Sugars | 0.087 - 0.22 | ||
Tantalum | |||
Tar | 0.19 | ||
Tellurium | 4.9 | ||
Thorium | |||
Timber, alder | 0.17 | ||
Timber, ash | 0.16 | ||
Timber, birch | 0.14 | ||
Timber, larch | 0.12 | ||
Timber, maple | 0.16 | ||
Timber, oak | 0.17 | ||
Timber, pitchpine | 0.14 | ||
Timber, pockwood | 0.19 | ||
Timber, red beech | 0.14 | ||
Timber, red pine | 0.15 | ||
Timber, white pine | 0.15 | ||
Timber, walnut | 0.15 | ||
Tin | |||
Titanium | |||
Tungsten | |||
Uranium | |||
Urethane foam | 0.021 | ||
Vacuum | 0 | ||
Vermiculite granules | 0.065 | ||
Vinyl ester | 0.25 | ||
Water | 0.606 | ||
Water, vapor (steam) | 0.0267 | 0.0359 | |
Wheat flour | 0.45 | ||
White metal | 35 - 70 | ||
Wood across the grain, white pine | 0.12 | ||
Wood across the grain, balsa | 0.055 | ||
Wood across the grain, yellow pine, timber | 0.147 | ||
Wood, oak | 0.17 | ||
Wool, felt | 0.07 | ||
Wood wool, slab | 0.1 - 0.15 | ||
Xenon (gas) | 0.0051 | ||
Zinc |
1) Asbestos is bad for human health when the tiny abrasive fibers are inhaled into the lungs where they can damage the lung tissue. This seems to be exacerbated by cigarette smoking and the resulting diseases are mesothelioma and lung cancer.
- 1 W/(m K) = 1 W/(m o C) = 0.85984 kcal/(h m o C) = 0.5779 Btu/(ft h o F) = 0.048 Btu/(in h o F) = 6.935 (Btu in)/(ft² h °F)
- Thermal Conductivity - Unit Converter
- What is conductive heat transfer?
Example - Conductive Heat Transfer through an Aluminum Pot versus a Stainless Steel Pot
The conductive heat transfer through a pot wall can be calculated as
q = (k / s) A dT (1)
or alternatively
q / A = (k / s) dT
where
q = heat transfer (W, Btu/h)
A = surface area (m 2 , ft 2 )
q / A = heat transfer per unit area (W/m 2 , Btu/(h ft 2 ))
k = thermal conductivity (W/mK, Btu/(hr ft °F))
dT = t 1 - t 2 = temperature difference ( o C, o F)
s = wall thickness (m, ft)
Conductive Heat Transfer Calculator
Note! - that the overall heat transfer through a surface is determined by the " overall heat transfer coefficient " - which in addition to conductive heat transfer - depends on
- the convective heat transfer coefficients on the inside and outside of the surfaces
- the radiant heat transfer coefficients on the inside and outside of the surfaces
Conductive Heat Transfer through an Aluminum Pot Wall with thickness 2 mm - temperature difference 80 o C
Thermal conductivity for aluminum is 215 W/(m K) (from the table above). Conductive heat transfer per unit area can be calculated as
q / A = [(215 W/(m K)) / (2 10 -3 m)] (80 o C)
= 86 00000 (W/m 2 )
= 8600 (kW/m 2 )
Conductive Heat Transfer through a Stainless Steel Pot Wall with thickness 2 mm - temperature difference 80 o C
Thermal conductivity for stainless steel is 17 W/(m K) (from the table above). Conductive heat transfer per unit area can be calculated as
q / A = [(17 W/(m K)) / (2 10 -3 m)] (80 o C)
= 680000 (W/m 2 )
= 680 (kW/m 2 )
Related Topics
-
Insulation
Heat transfer and heat loss from buildings and technical applications - heat transfer coefficients and insulation methods to reduce energy consumption. -
Material Properties
Material properties of gases, fluids and solids - densities, specific heats, viscosities and more. -
Thermodynamics
Work, heat and energy systems.
Related Documents
-
Aluminum Alloys - Mechanical Properties
Mechanical properties of aluminum alloys - tensile strength, yield strength and more. -
Brick Densities
Densities of common types of bricks. -
Butane - Thermal Conductivity vs. Temperature and Pressure
Online calculators, figures and tables showing thermal conductivity of liquid and gaseous butane, C4H10, at varying temperature and pressure, SI and Imperial units. -
Calcium Silicate Insulation
Thermal conductivity of calcium silicate insulation - temperature and k-values. -
Carbon dioxide - Prandtl Number vs. Temperature and Pressure
Figures and table with changes in Prandtl number for carbon dioxide with changes in temperature and pressure. -
Carbon Dioxide - Thermophysical Properties
Chemical, physical and thermal properties of carbon dioxide. Phase diagram included. -
Conductive Heat Transfer
Conductive heat transfer takes place in a solid if there is a temperature gradient. -
Ethane - Thermal Conductivity vs. Temperature and Pressure
Online calculator, figures and table showing thermal conductivity of ethane, C2H6, at varying temperature and pressure - Imperial and SI Units. -
Ethylene - Thermal Conductivity vs. Temperature and Pressure
Online calculator, figures and table showing thermal conductivity of ethylene, also called ethene or acetene, C2H4, at varying temperature and pressure - Imperial and SI Units. -
Foods - Thermal Conductivities
Thermal conductivity of selected foodstuff like apples, beef, sugar and more. -
Heat Exchanger Materials - Thermal Conductivities
Typical heat exchanger materials and their thermal conductivities. -
Hydrogen - Thermal Conductivity vs. Temperature and Pressure
Online calculator, figures and table showing thermal conductivity of hydrogen, H2, at varying temperature and pressure - Imperial and SI Units. -
Insulation Materials - Operating Temperature Limits
Temperature limits for commonly used insulation materials. -
Liquids - Thermal Conductivities
Some fluids and their thermal conductivities. -
Metals, Metallic Elements and Alloys - Thermal Conductivities
Thermal conductivities of common metals, metallic elements aand alloys. -
Mineral Wool Insulation
Thermal conductivity - k-values - vs. temperature. -
Mortar Types
ASTM mortar types. -
Nitrogen - Thermal Conductivity vs. Temperature and Pressure
Online calculator, figures and tables showing thermal conductivity of nitrogen, N2, at varying temperarure and pressure, SI and Imperial units. -
Overall Heat Transfer Coefficients
Walls or heat exchangers - calculate overall heat transfer coefficients. -
Pipes and Cylinders - Conductive Heat Losses
Conductive heat losses through cylinder or pipe walls. -
Plastics - Thermal Conductivity Coefficients
Thermal conductivity of plastics. -
Propane - Thermal Conductivity vs. Temperature and Pressure
Online calculator, figures and tables showing thermal conductivity of liquid and gaseous propane at varying temperarure and pressure, SI and Imperial units. -
Thermal Conductivity - Online Converter
Convert between thermal conductivity units. -
Thermal Conductivity - Unit Converting Table
Convert between thermal conductivity units - table and diagram. -
Thermal Resistivity and Conductivity
The ability of a material to resist flow of heat. -
Thermal Transmittance vs. Thermal Resistance
The thermal transmittance U vs. the thermal resistance R. -
Water - Thermal Conductivity vs. Temperature
Figures and tables showing thermal conductivity of water (liquid and gas phase) with varying temperature and pressure, SI and Imperial units.